• Welcome to ClassicBroncos! - You are currently viewing the forums as a GUEST. To take advantage of all the site features, please take a moment to register. It's fast, simple and absolutely free. So please join our community today!
    If you have problems registering or can't log into your account, please contact Admin.

Pitted panels

Mac2Night

Bronco Guru
Joined
Aug 10, 2005
Messages
2,204
So I am stepping into an area that I am uncertain about, but I know someone here has the answer.

I have a grille that is in great shape (solid and straight) other than being pitted (the nose of the truck stuck out from under a shed for 20+ years. The metal is solid and not scaly with flaking rust at all but it is bumpy with pits. Will sand or media blasting take the pitting out and if not, what are my options?

Once I get some or all of the pitting out, can I skim the remaining defects and sand to make the grille usable?

Thanks, Mac
 

Attachments

  • Screen Shot 2016-01-25 at 4.22.23 PM.jpg
    Screen Shot 2016-01-25 at 4.22.23 PM.jpg
    83.5 KB · Views: 101
  • Screen Shot 2016-01-25 at 4.22.41 PM.jpg
    Screen Shot 2016-01-25 at 4.22.41 PM.jpg
    38.4 KB · Views: 100
Last edited:

kip60

Full Member
Joined
Feb 7, 2015
Messages
239
Sand blasting or media will probably just make it worse. I would take some aggressive sanding disk and level it out a bit, then like Fordguy said, level it up with primer and/or skim coat, and sand it smooth.
 

Apogee

Contributor
Bronco Guru
Joined
Nov 26, 2005
Messages
6,349
Loc.
Tangent, OR
High build primer or a skim coat (1/32") of plastic filler.

Multiple coats of high-build primer might get you where you want to be, or any of the usual filler options...I'm not sure what the practical limits are there. My inclination would be to hit it with a few coats of high-build primer, sanding off the high spots, rinsing and repeating until I had the results I wanted.
 

broncosbybart

Bronco Guru
Joined
Mar 13, 2002
Messages
2,644
Blasting will make it worse. After sanding, I'd use epoxy on it before using a 2k. If the pits are too deep (looks like they are), glazing puddy would work well. Depending on where the pits are, it could be more work than it's worth. Grilles take a lot of time to fix.
 

JAFO

Bronco Guru
Joined
Dec 3, 2007
Messages
1,556
Loc.
Beaverdam
You just don't want rust to bleed through. Make sure the pitting isn't still rust. Maybe a wire wheel on the grinder all over the pitting. You could check the various rust converter products at say Eastwood.com to see if they recommend anything that could convert the rust but be safely painted.
 

Apogee

Contributor
Bronco Guru
Joined
Nov 26, 2005
Messages
6,349
Loc.
Tangent, OR
You could etch it with Metal Ready or some similar acid product to make sure all of the pits are clear of rust before coating it.
 

grant_71

Bronco Guru
Joined
Aug 6, 2002
Messages
1,936
Electrolysis to remove the rust without making the pitting worse (like media blasting would), then sand the high spots of the pitting down just a bit to smooth it out. Then etch prime, and high build prime. Sand, prime, fill repeat....
 
Top